Epoxy adhesion over stains

We have occasionally reported results of adhesion testing of WEST SYSTEM® epoxy to wood coated with various stains. In "Varnish over epoxy" in Epoxyworks 18, we touched on the topic of wood stains under epoxy and warned that some oil-based stains would cause an adhesion problem for WEST SYSTEM epoxy. Since then, we have done some additional adhesion testing to a number of stains (below).


These included paste wood filler stain, oil-based stains and water-based stains. This testing also compared adhesion of epoxy to stains that had dried one day to stains that had dried four days. We tested adhesion using our variation of ASTM-3359-83, which involves scoring the epoxy coating with a razor blade. Two to three 2" long cuts are made parallel to one another about ¼" apart, deep enough to pass through the epoxy. Another set of cuts is made to intersect the first at a 45° to 90° angle. The points of intersection create ideal places where the epoxy coating will peel off if adhesion is poor. In the ASTM test, a special 3M™ tape with high tack is applied over the scored area and pressed into the coating to assure thorough contact. We substituted quality duct tape with high tack strength for the 3M tape.


Once applied, the tape is pulled back at a flat angle, quickly, with a firm tug. If adhesion is poor, the epoxy will peel from the surface and remain attached to the tape (above). If adhesion is good, the epoxy remains attached to the stained surface.

Test results

Stain brand/type 24 hr. dry 4-day dry
Pettit™ Paste Wood Filler Stain fail (see photo) pass
Minwax™ Wood Finish (oil base) fail fail
Minwax Gel Stain pass pass
WD Lockwood™ water-base aniline dye stain pass pass
Minwax water-base stain pass pass
Pratt & Lambert™ Tonetic oil-base stain pass pass
Old Masters™ oil-base (wiping) stain pass pass
Ace Brand™ oil-base stain pass pass
Bare wood control pass pass

These results show that WEST SYSTEM epoxy adheres to some oil-base stains after 24 hours of drying. Others require more drying time before epoxy will adhere reliably. Our epoxy did not stick to Minwax Wood Finish even after four days of drying under ideal drying conditions.

If you have a preferred stain not listed above, you can conduct your own adhesion test. Be sure to cut completely through the epoxy coating and use a high tack tape. If you have no preferred stain, consider WD Lockwood's (212-966-4046) water-based aniline dye stain. It has worked reliably under epoxy for many years. -Tom Pawlak

Epoxyworks 21 / Summer 2003

Copyright © 2003, Gougeon Brothers, Inc. All rights reserved.
This page is maintained by Gougeon Brothers, Inc. Last modified on (11/05/03).
Reproduction in any form, in whole or in part, is expressly forbidden without the consent of the publisher. EPOXYWORKS, Gougeon Brothers, WEST SYSTEM, Episize, Scarffer and Microlight as used throughout this publication, are trademarks of Gougeon Brothers, Inc., Bay City, Michigan, USA.